论文部分内容阅读
研究了大足中低品位天青石矿的工艺矿物学特性,该矿石天青石与主要脉石矿物在物性上的最大差异是密度;进行了重选试验,采用跳汰-摇床的工艺,可以把原矿品位为69.75%的天青石矿分达成品位为92.44%的优质精矿,回收率为82.43%;生产实践取得了较好指标,达到或超过设计指标,证明了试验所选取的条件是正确的,工艺是合理的。
The technological mineralogical characteristics of mid-low-grade celestite from Dazu were studied. The biggest difference in physical properties between the celestite and the main gangue minerals was the density. The re-election test was conducted using the technology of jig-shaker Raw ore grade of 69.75% celestite ore reached grade of 92.44% quality grade concentrate, the recovery rate was 82.43%; production practice has made a good indicator to meet or exceed the design indicators that the test Select the conditions are correct, the process is reasonable.